s*****n 发帖数: 741 | 1 I recently coated a PTFE (poly tetra fluoro ethylene) device with some
methacrylat. The coating layer gave round disk like uncontinued morphology
on the device surface, we need get even surface.
I used simple coat method, dip the device into the mehacrylate monomer/
initiator solution, take it out and let the monomer polymerize on the device
surface.
Any suggestions? Thanks in advance, do you think spin coating would help? or
any other coating method? |
l*****g 发帖数: 556 | 2 Plasma or Corona surface activation.
Then CVD deposition?
device
or
【在 s*****n 的大作中提到】 : I recently coated a PTFE (poly tetra fluoro ethylene) device with some : methacrylat. The coating layer gave round disk like uncontinued morphology : on the device surface, we need get even surface. : I used simple coat method, dip the device into the mehacrylate monomer/ : initiator solution, take it out and let the monomer polymerize on the device : surface. : Any suggestions? Thanks in advance, do you think spin coating would help? or : any other coating method?
|
s*****n 发帖数: 741 | 3 Thanks for answering, could you please give some papers or links for me to
learn the techniques you mentioned? |
t****1 发帖数: 232 | 4 You could polymerize first in the solvent (not a good solvent for PTFE) and
the polymer MW is controllable. Then spray the polymer solution on the
surface of PTFE and evaporate the solvent. |
z*****7 发帖数: 133 | 5 coat sth onto PTFE is technically difficult due to the surface tension of
PTFE.
physical/chemical etching is necessary according to published articles. |
s*****n 发帖数: 741 | 6 problem solved, thanks you all. |
a*i 发帖数: 1652 | 7 怎么解决的? 是不是让器件不停旋转?
【在 s*****n 的大作中提到】 : problem solved, thanks you all.
|